← All theory chapters
Theory / Mechanics & Materials

From Tensile Data to a Plasticity Input Curve

Convert measured quantities carefully and preserve the limits of the test.

Theory · Educational notes · Related tools: Abaqus · LS-DYNA

Which strain belongs in a plastic material card?

At a uniform tensile point, engineering stress is 300 MPa and engineering strain is 0.05. Use E = 200000 MPa to convert to true stress and logarithmic plastic strain.

The stress conversion accounts approximately for area change. Logarithmic total strain still includes elastic strain, which the solver will compute separately. Subtract that elastic part before preparing a plastic-strain table; after necking the uniform conversion is no longer sufficient.

Connect the physical quantities

Engineering stress uses original area; true stress uses current area. The familiar conversion assumes uniform deformation and an approximate volume relation. Once necking starts, a single global extension no longer specifies the local strain or current neck area.

The relationship used in this example

εln⁡p=εln⁡−σtrueE\varepsilon_{\ln}^{p}=\varepsilon_{\ln}-\frac{\sigma_{\mathrm{true}}}{E}

Engineering stress uses the original area; true stress uses the current area. Logarithmic strain measures incremental stretch. Many classical metal models require true yield stress against plastic strain, rather than the total engineering strain reported by a test machine.

Work through the example

Step 1

Convert stress: 300(1+0.05) = 315 MPa.

Step 2

Logarithmic total strain is ln(1.05) = 0.0487902.

Step 3

Subtract elastic strain 315/200000 = 0.001575 to obtain plastic strain 0.0472152.

Full example conditions and reference values

At a synthetic uniform-deformation test point, engineering stress is 300 MPa and engineering strain is 0.05. With E = 200,000 MPa, the usual constant-volume approximation gives true stress 315 MPa, logarithmic strain 0.0487902 and plastic strain 0.0472152. This one point is not a complete material curve; the initial yield point and remaining measured range must also be defined.

Compare the numbers before judging the result

Compare the calculated values
ConditionValue
Engineering strain0.05
Logarithmic total strain0.04879016
Elastic part0.001575
Plastic input0.04721516

Only the last value belongs in the plastic-strain coordinate for this converted point.

What the result means for a model

The first plastic-table point normally corresponds to initial yield at zero plastic strain for this convention. Inspect units, monotonicity and extrapolation. Do not extend the uniform-deformation conversion through necking and claim calibrated local fracture behavior.

Keep the measured engineering curve and converted curve separately. After necking, uniform-area conversion no longer reconstructs the local material law; use local measurements or an inverse method appropriate to the specimen and stress state.

Another application: Why the first plastic-strain point matters

At the example point, total logarithmic strain is 0.0487902 and elastic strain is 315/200000 = 0.001575. The plastic input is their difference, 0.0472152. The initial yield entry has zero plastic strain; it is not the zero-stress origin of the tensile test.

Further modeling details

Preserve raw evidence

Keep force, gauge displacement or strain, initial dimensions, specimen orientation, temperature and loading rate. Store each transformation separately so the material input can be traced back to the test.

Build the table

Use consistent units and strain fractions, not percentages. Identify the model’s initial yield definition and set its reference plastic strain consistently. Check ordering, repeated points, smoothing and interpolation. Keep the original curve beside the processed table.

Beyond uniform tension

After necking, local area and strain measurements or inverse identification are normally needed. Match the specimen force–displacement and deformation field rather than extending a conversion formula without evidence.

Validate the exported input

Reproduce the test with a simple specimen model. Review stiffness, yield, plastic range and unloading separately. State extrapolation beyond the measured range and avoid treating an assumed tail as measured data.

Formula and symbol reference

Open the complete formula reference
σeng=FA0\sigma_{\mathrm{eng}}=\frac{F}{A_0}
σtrue≈σeng(1+εeng)\sigma_{\mathrm{true}}\approx\sigma_{\mathrm{eng}}(1+\varepsilon_{\mathrm{eng}})
εln⁡=ln⁡(1+εeng)\varepsilon_{\ln}=\ln(1+\varepsilon_{\mathrm{eng}})
εln⁡p=εln⁡−σtrueE\varepsilon_{\ln}^{p}=\varepsilon_{\ln}-\frac{\sigma_{\mathrm{true}}}{E}
SymbolMeaningUnit / convention
F, A0Force; initial cross-sectional areaN; mm²
σeng, σtrueEngineering and true stressMPa
εeng, εlnEngineering and logarithmic total straindimensionless
εlnᵖApproximate logarithmic plastic strain for small elastic straindimensionless

When this example stops applying

The stress conversion assumes uniform deformation and approximately constant volume; elastic compressibility is neglected. It is not valid as a general post-necking conversion. Machine crosshead displacement may contain grip or fixture compliance. A negative computed plastic strain requires investigation, not blind clipping.

Check your interpretation

Can the descending engineering-stress curve after necking be copied directly as constitutive softening?

Show the reasoning

No. The measured force reduction includes geometric localization and cannot by itself identify a local material softening law.

Sources and calculation scope

The questions and comparison tables are independently authored teaching examples. Numbers illustrate the stated models; they are not measured cell/pack data or commercial-solver validation.

Comparison calculations (Python)

English / Korean · revised 1 November 2026