← All theory chapters
Theory / Mechanics & Materials

Pad Relaxation, Creep & Repeated Compression

Distinguish held-displacement relaxation from held-force creep, then interpret unloading and recovery.

Theory · Educational notes

Why do a held force and a held gap give different curves?

Use a standard linear solid with k0 = 1000 N/mm, k∞ = 400 N/mm and relaxation time 60 s. Compare holding 0.10 mm compression with holding 100 N force.

At fixed compression, internal redistribution reduces force: relaxation. At fixed force, the same redistribution allows more compression: creep. The boundary condition changes which variable evolves, and the creep time constant is not generally the relaxation time constant.

Connect the physical quantities

The relationship used in this example

F(t)=δ0kR(t)F(t)=\delta_0 k_R(t)

A static compression curve does not describe what happens during a long hold. At fixed compression, force may relax; at fixed force, compression may increase. The boundary being held is therefore part of the material experiment. A simple standard linear solid provides a useful first comparison before nonlinear foam, temperature and permanent-set effects are introduced.

Work through the example

Step 1

Held displacement: F(60) = 0.10[400+600 exp(−1)] = 62.073 N.

Step 2

Held force: τC = 60×1000/400 = 150 s; δ(60) = 100[1/400−(1/400−1/1000)exp(−60/150)] = 0.149452 mm.

Step 3

Remove force at 150 s: at t = 300 s use 100[J(300)−J(150)] = 0.034882 mm. It is delayed recovery, not permanent set.

Full example conditions and reference values

Synthetic standard linear solid: k₀ = 1000 N/mm, k∞ = 400 N/mm and τR = 60 s. Case A holds compression at 0.10 mm: force starts at 100 N, is 62.073 N at 60 s and approaches 40 N. Case B instead holds force at 100 N: τC = 150 s, compression starts at 0.10 mm, reaches 0.149452 mm at 60 s and approaches 0.25 mm. These are separate boundary conditions on the same illustrative model.

Pad Relaxation, Creep & Repeated Compression — synthetic analytical example
Original Jaylab analytical illustration. Synthetic inputs; not a measured battery or pack response.

Compare the numbers before judging the result

Compare the calculated values
Time (s)Held 0.10 mm: force (N)Held 100 N: compression (mm)
01000.1
6062.072770.149452
15044.92510.1948181
60040.002720.2472527

Columns describe independent boundary-condition tests, not simultaneous force and displacement on one specimen.

What the result means for a model

Use the pad’s time-dependent constitutive law inside assembly compatibility. Keep temperature and loading history consistent; a short compression test cannot identify long-term relaxation or permanent set by itself.

Another application: A real stack is between ideal hold conditions

At 60 s, the ideal fixed-displacement case retains 62.073 N, while the independent fixed-force case reaches 0.149452 mm. These results belong to different tests. A compliant housing allows both force and pad compression to evolve, so neither ideal curve can be copied directly into the assembled response.

Further modeling details

Read the boundary before the curve

A crosshead held still does not guarantee a fixed local pad thickness if the frame, load cell or specimen seating changes. Record both local displacement and force during the hold. For a pad in a cell–frame assembly, neither local force nor local displacement is generally constant; solve compatibility with the other components.

Build the smallest time-dependent model

The standard linear solid places an equilibrium spring in parallel with a Maxwell spring–dashpot branch. Under a displacement step, the branch force decays while the equilibrium spring still carries load. The formulas describe a uniform axial element; they are not a complete three-dimensional pad material card.

Do not take creep as the reciprocal of relaxation

J(t) is not 1/kR(t) at every time. For this model, τC/τR = k₀/k∞ = 2.5. Using the same time constant for both experiments would give the wrong transient even though the initial and final limits might agree. Compare the entire curve and its loading protocol.

Unloading separates delayed recovery from permanent set

In Case B, remove the 100 N force at th = 150 s. Compression immediately before release is 0.194818 mm; an elastic recovery of 0.10 mm leaves 0.094818 mm immediately after release. It falls to 0.034882 mm at t = 300 s and tends to zero. Residual compression shortly after unloading is therefore not proof of permanent set. This ideal solid has no permanent deformation.

Repeated compression requires history

For linear viscoelasticity, successive force steps can be superposed with their own start times. Restarting every cycle from a fresh material state erases delayed recovery. Measured cycle-to-cycle changes may additionally need plasticity, foam damage, Mullins effects or temperature dependence; one linear relaxation time cannot represent all of them.

Plan an identifiable experiment

Use several hold durations around the observed relaxation times, a recorded loading ramp, recovery time and repeat specimens. Keep temperature and contact friction controlled. Fit relaxation and then predict a different hold or creep case without retuning. A long-term stiffness cannot be confidently identified from a test that ends before a plateau is approached.

Transfer to a solver carefully

Convert axial stiffness to material properties only with justified area, thickness and lateral constraints. A measured compression response is not automatically a shear-relaxation Prony series. Use the solver’s required instantaneous/equilibrium convention, shear and volumetric data, and a single-element reproduction of the measured protocol before the assembly model.

Formula and symbol reference

Open the complete formula reference
kR(t)=k∞+(k0−k∞)e−t/τRk_R(t)=k_\infty+(k_0-k_\infty)e^{-t/\tau_R}
F(t)=δ0kR(t)F(t)=\delta_0 k_R(t)
J(t)=1k∞−(1k∞−1k0)e−t/τCJ(t)=\frac{1}{k_\infty}-\left(\frac{1}{k_\infty}-\frac{1}{k_0}\right)e^{-t/\tau_C}
δ(t)=F0J(t),τC=k0k∞τR\delta(t)=F_0J(t),\qquad\tau_C=\frac{k_0}{k_\infty}\tau_R
δ(t)=F0[J(t)−J(t−th)](t≥th)\delta(t)=F_0[J(t)-J(t-t_h)]\quad(t\geq t_h)
SymbolMeaningUnit / convention
k₀, k∞Instantaneous and equilibrium axial stiffness; k₀ > k∞ > 0N/mm
τR, τCRelaxation and creep time constants of this standard linear solids
J, δ, FAxial creep compliance, compression and forcemm/N; mm; N
thTime at which the applied force is removeds

When this example stops applying

Small-strain, linear, isothermal axial model with ideal step loading and constant geometry. The recovery example is force controlled. A prescribed return to zero compression may require tensile reaction and cannot be applied blindly to an unbonded compression-only pad. No densification, plastic set or actual pad calibration is claimed.

Check your interpretation

Does nonzero compression immediately after unloading prove permanent damage?

Show the reasoning

No. Delayed viscoelastic recovery can leave a temporary residual. Observe a sufficiently long recovery under a defined boundary and distinguish it from permanent set.

Sources and calculation scope

The questions and comparison tables are independently authored teaching examples. Numbers illustrate the stated models; they are not measured cell/pack data or commercial-solver validation.

Comparison calculations (Python)

English / Korean · revised 1 November 2026